   FRP structural shapes profile is made of glass fiber reinforced material, resin as adhesive, glass fiber cloth as a package reinforcement layer, through the thorough penetration, in the metal mold heating, molding, curing, drawing in the traction machine pulled A new type of composite material, with good physical properties, widely used in high strength, large span Situation.   

Large wave corrugated board

Varieties

Size(mm)

Weight(kg/m)

Size(in)

Weight(lbs/in)


1000*50.8*49.1

39" x 2" x 3/16"

20.1

Markets  

Markets

  • Architectural

  • Bridge & Highway

  • Chemical

  • Food & Beverage

  • Manufacturing

  • Metals & Mining

  • Microelectronics

  • Oil & Gsa

  • Pharmaceutical

  • Power

  • Pulp & Paper

  • Recreation

  • Telecommunications

  • Transportation

  • Water & Wastewater

The characteristics:

  • Corrosion Resistant

  • Low Maintenance

  • Fire Retardant

  • Low Install Cost

  • Heavy Metal Safe

  • Long Service Life

  • Electrically & Thermally Non Conductive

  • High Strength-to-Weight Ratio

Introduction of raw materials——Resin type

Code

Resin type

Flame retardant property

Recommended usage occasions

VEFR-25

Vinyl type

Oxygen index 28 or above

Acid, alkali and other corrosive harsh environment

IFR-25

Meta benzene

Oxygen index 28 or above

A VEFR type economy, and excellent, moderate acid alkali and solvent

OFR-25

Ortho type

Oxygen index 28 or above

General acid and alkali environment

 Application:  

   Genius© pultruded fiberglass structural shapes from Genius Composite Inc. are used in a wide range of applications and provide a unique combination of corrosion resistance, high strength, dimensional stability and light weight, along with thermal and electric non-conductivity. Durable Genius shapes provide years of low maintenance service in areas where steel, aluminum or wood components are traditionally specified. Today ,these shapes are often used in highly corrosive applications where stainless steel and other expensive components were once required.  

Genius Shapes

Mechanical Properties

ASTM

Units

Value

Units

Value

Tensile Stress, LW

D-638

psi

30000

kgf/m²

21092086

Tensile Stress, CW

D-638

psi

7000

kgf/m²

4921487

Tensile Modulus, LW

D-638

10^6psi

2.5

10^6kgf/m²

1758

Tensile Modulus, CW

D-638

10^6psi

0.8

10^6kgf/m²

562

Compressive Stress, LW

D-695

psi

30000

kgf/m²

21092086

Compressive Stress, CW

D-695

psi

15000

kgf/m²

10546043

Compressive Modulus, LW

D-695

10^6psi

2.5

10^6kgf/m²

1758

Compressive Modulus, CW

D-695

10^6psi

1

10^6kgf/m²

703

Flexural Stress, LW

D-790

psi

30000

kgf/m²

21092086

Flexural Stress, CW

D-790

psi

10000

kgf/m²

7030695

Flexural Modulus, LW

D-790

10^6psi

1.8

10^6kgf/m²

1266

Flexural Modulus, CW

D-790

10^6psi

0.8

10^6kgf/m²

562

Modulus of Elasticity

Full Section

10^6psi

2.8

10^6kgf/m²

1969

Shear Modulus

---

10^6psi

0.45

10^6kgf/m²

316

Short Beam Shear

D-2344

psi

4500

kgf/m²

3163813

Punch Shear

D-732

psi

10000

kgf/m²

7030695

Notched Izod Impact,LW

D-256

ft.-lbs./in.

25

kg/m

3.46

Notched Izod Impact,CW

D-256

ft.-lbs./in.

4

kg/m

0.55

  Excludes Round Rod and Square Bar

Physical Properties

ASTM

Units

Value

Barcoal

D-495

---

45

24 Hour Water Absorption

D-570

%max

0.45

Density

D-792

lbs./in.³

0.062-0.07

Coefficient of Thermal Expansion,LW

D-696

10^-6in./in./℃

8

Flammability Properties

ASTM

Units

Value

Tunnel test*

E-84

Flame Spread

25 max

Flammability*

D-635

---

Non-Burning

Electrical Properties

ASTM

Units

Value

Arc Resistance,LW

D-495

seconds

120

Dielectric Strength,LW

D-149

kv./in.

35

Dielectric Strength,PF

D-149

volts/mil

200

Dielectric Constant,PF

D-150

@60hz

5

LW=Lengthwise, CW=Crosswise,PF=Perpendicular to Laminate Face

*Pertains to ISOFR and VEFR only


Application Scenarios

Large corrugated sheets are commonly used for roof and wall cladding of industrial plants, warehouses, chemical plants, sewage tanks and similar buildings. They can also be used for outdoor sun shading, canopies and equipment protective covers with high corrosion resistance requirements. The vinyl resin provides good chemical corrosion resistance and weather resistance, making it suitable for corrosive gas or humid environments. To learn about suitability for specific working conditions, please contact us for detailed specifications and recommendations.

Selection Guide

During selection, load, span, support spacing and the corrosion level of the service environment should be considered comprehensively to determine the appropriate sheet thickness, corrugation and length. Large corrugated sheets usually adapt to different spans by adjusting overlap and fixing methods. Structural calculation by a professional engineer is recommended. We can provide customized solutions based on your project requirements. Please contact us for detailed specifications and quotations.

Product Advantages

This product uses glass fiber reinforced vinyl resin and is pultruded, featuring light weight, high strength, corrosion resistance, aging resistance and adjustable light transmission (requiring corresponding additives), and is easy to cut and install with low maintenance cost. Compared with metal sheets, it has a longer service life in corrosive environments and good insulation performance. To compare with other materials or learn specific performance data, please contact us for detailed specifications and quotations.

Inquiry Guide

To obtain detailed technical parameters, samples or quotations for large corrugated sheets, please provide your specific application scenario, dimension requirements and quantity. Our technical team will provide selection support. Please contact us for detailed specifications and quotations.

Operating Environment

  • This molded vinyl ester FRP corrugated structural profile is designed for both indoor and outdoor installations, including industrial plants, chemical processing areas, and architectural applications where the material's vinyl ester resin matrix provides resistance to moisture and humidity.
  • The vinyl ester resin used in this FRP structural shape offers enhanced tolerance to a range of corrosive media, including many acids, alkalis, and salt solutions, making it suitable for environments where steel or other metals would degrade rapidly.
  • Typical service conditions include exposure to temperature fluctuations; the material's physical properties are stable across common ambient and industrial operating temperature ranges, though specific limits depend on the exact chemical environment and load requirements.
  • This product line is frequently specified for high-strength, large-span situations in sectors such as architectural, bridge & highway, chemical, food & beverage, manufacturing, metals & mining, and microelectronics, where durability against weather, humidity, and chemical attack is essential.

立即联系我们,我们将有专业人员为您服务。

7*24 professional team support. Within 24 Hours, our team will give you the feedback.

Send