   FRP structural shapes profile is made of glass fiber reinforced material, resin as adhesive, glass fiber cloth as a package reinforcement layer, through the thorough penetration, in the metal mold heating, molding, curing, drawing in the traction machine pulled A new type of composite material, with good physical properties, widely used in high strength, large span Situation.   

Hollow board

Varieties

Size(mm)

Weight(kg/m)

Size(in)

Weight(lbs/in)

Hollow board

A1*T1*A2*T2*B*T3
A1*T1*A2*T2*B*T3

500*6*450*6*48.5*616.4

20" x 1/4" x 18" x 1/4" x 2" x 1/4"

36.2

500*6*450*6*48.5*918.5

20" x 1/4" x 18" x 1/4" x 2" x 3/8"

40.8

650*13*550*13*98.5*1252.5

51/2" x 1/2" x 173/8" x 1/2" x 4" x 1/2"

116

725*4.5*675*4.5*45*4.517.9

57/2" x 3/16" x 53/2" x 3/16" x 7/4" x 3/16"

39.5

Markets  

Markets

  • Architectural

  • Bridge & Highway

  • Chemical

  • Food & Beverage

  • Manufacturing

  • Metals & Mining

  • Microelectronics

  • Oil & Gsa

  • Pharmaceutical

  • Power

  • Pulp & Paper

  • Recreation

  • Telecommunications

  • Transportation

  • Water & Wastewater

The characteristics:

  • Corrosion Resistant

  • Low Maintenance

  • Fire Retardant

  • Low Install Cost

  • Heavy Metal Safe

  • Long Service Life

  • Electrically & Thermally Non Conductive

  • High Strength-to-Weight Ratio

Introduction of raw materials——Resin type

Code

Resin type

Flame retardant property

Recommended usage occasions

VEFR-25

Vinyl type

Oxygen index 28 or above

Acid, alkali and other corrosive harsh environment

IFR-25

Meta benzene

Oxygen index 28 or above

A VEFR type economy, and excellent, moderate acid alkali and solvent

OFR-25

Ortho type

Oxygen index 28 or above

General acid and alkali environment

 Application:    

   Genius© pultruded fiberglass structural shapes from Genius Composite Inc. are used in a wide range of applications and provide a unique combination of corrosion resistance, high strength, dimensional stability and light weight, along with thermal and electric non-conductivity. Durable Genius shapes provide years of low maintenance service in areas where steel, aluminum or wood components are traditionally specified. Today ,these shapes are often used in highly corrosive applications where stainless steel and other expensive components were once required.    

Genius Shapes

Mechanical Properties

ASTM

Units

Value

Units

Value

Tensile Stress, LW

D-638

psi

30000

kgf/m²

21092086

Tensile Stress, CW

D-638

psi

7000

kgf/m²

4921487

Tensile Modulus, LW

D-638

10^6psi

2.5

10^6kgf/m²

1758

Tensile Modulus, CW

D-638

10^6psi

0.8

10^6kgf/m²

562

Compressive Stress, LW

D-695

psi

30000

kgf/m²

21092086

Compressive Stress, CW

D-695

psi

15000

kgf/m²

10546043

Compressive Modulus, LW

D-695

10^6psi

2.5

10^6kgf/m²

1758

Compressive Modulus, CW

D-695

10^6psi

1

10^6kgf/m²

703

Flexural Stress, LW

D-790

psi

30000

kgf/m²

21092086

Flexural Stress, CW

D-790

psi

10000

kgf/m²

7030695

Flexural Modulus, LW

D-790

10^6psi

1.8

10^6kgf/m²

1266

Flexural Modulus, CW

D-790

10^6psi

0.8

10^6kgf/m²

562

Modulus of Elasticity

Full Section

10^6psi

2.8

10^6kgf/m²

1969

Shear Modulus

---

10^6psi

0.45

10^6kgf/m²

316

Short Beam Shear

D-2344

psi

4500

kgf/m²

3163813

Punch Shear

D-732

psi

10000

kgf/m²

7030695

Notched Izod Impact,LW

D-256

ft.-lbs./in.

25

kg/m

3.46

Notched Izod Impact,CW

D-256

ft.-lbs./in.

4

kg/m

0.55

  Excludes Round Rod and Square Bar  

Physical Properties

ASTM

Units

Value

Barcoal

D-495

---

45

24 Hour Water Absorption

D-570

%max

0.45

Density

D-792

lbs./in.³

0.062-0.07

Coefficient of Thermal Expansion,LW

D-696

10^-6in./in./℃

8

Flammability Properties

ASTM

Units

Value

Tunnel test*

E-84

Flame Spread

25 max

Flammability*

D-635

---

Non-Burning

Electrical Properties

ASTM

Units

Value

Arc Resistance,LW

D-495

seconds

120

Dielectric Strength,LW

D-149

kv./in.

35

Dielectric Strength,PF

D-149

volts/mil

200

Dielectric Constant,PF

D-150

@60hz

5

LW=Lengthwise, CW=Crosswise,PF=Perpendicular to Laminate Face

*Pertains to ISOFR and VEFR only


Application Scenarios

Structural Profiles - Hollow Profile (Isophthalic) is suitable for load-bearing and supporting structures with requirements on strength and span, such as platform walkways, stair treads, handrails, cable tray supports, and frame members in corrosive environments such as chemical, marine engineering, and municipal applications. Its hollow cross-section maintains section stiffness while facilitating joining and drilled installation. To confirm whether it is suitable for your specific scenario, please contact us with your working conditions.

Selection Guide

During selection, first determine the section height and wall thickness based on span, load, and support method, then choose the drilling or joining solution according to the connection form of the installation joint; the isophthalic resin system is suitable for environments with high corrosion resistance requirements and can be further discussed based on media and temperature conditions. The specifications listed on the page are common references; for actual dimensions, weight, and mechanical parameters, please refer to the detailed specifications and quotation obtained by contacting us.

Product Advantages

This profile uses glass fiber as reinforcement and resin as matrix, and is formed by impregnation, heating, compression molding, and continuous pultrusion. It features lightweight, high strength, corrosion resistance, non-magnetic, electrical insulation, and ease of processing, cutting, and drilling. The hollow profile structure achieves a larger sectional moment of inertia with equal material usage, making it suitable for high-strength, large-span support needs. Please contact us for material system and process descriptions.

Inquiry Guidance

If you need to confirm requirements such as cross-section dimensions, length, color, surface treatment, and packaging and transportation, please contact us for detailed specifications and quotations. We will recommend suitable specifications and supply solutions based on your project conditions. Bulk procurement, custom cross-sections, and technical selection support can all be discussed together.

Free,easy click for support

7*24 professional team support. Within 24 Hours, our team will give you the feedback.

Send   
 Website Visitor