Product Category

Structural Profiles - H-Beam (Isophthalic)


Contact us for a quotation

Product details

Greenlogy TEC / Nantong Greenlogy Electronic Technology Co., Ltd.

  FRP pultruded profiles are a new composite material made with glass fiber reinforcement as the base material, resin as the adhesive, and glass fiber cloth as the wrapping reinforcement layer; after thorough impregnation, the material is heated, formed and cured in a metal mold and pulled by a pulling machine. It has good physical properties and is widely used in high-strength, long-span applications.  

Type

Size (mm)

Weight (kg/m)

Size (in)

Weight (lbs/in)

H-Beam

A*B*T1*T2


A*B*T1*T2


HB76

76*76*6.4*6.4

2.67

3" x 3" x 1/4" x 1/4"

5.73

HB102A

102*102*6.4*6.4

3.59

4" x 4" x 1/4" x 1/4"

7.91

HB102B

102*102*8*8

4.5

4" x 4" x 5/16" x 5/16"

9.92

HB152A

152*152*6.4*6.4

5.43

6" x 6" x 1/4" x 1/4"

11.97

HB152B

152*152*9.5*9.5

8.1

6" x 6" x 3/8" x 3/8"

17.86

HB203A

203*203*9.5*9.5

10.8

8" x 8" x 3/8" x 3/8"

23.81

HB203B

203*203*12.7*12.7

14.4

8" x 8" x 1/2" x 1/2"

31.66

HB203C

203*203*6.4*6.4

7.5

8" x 8" x 1/4" x 1/4"

16.53

HB254A

254*254*9.5*9.5

13.6

10" x 10" x 3/8" x 3/8"

29.98

HB254B

254*254*12.7*12.7

18

10" x 10" x 1/2" x 1/2"

39.77

HB305

305*305*12.7*12.7

21.5

12" x 12" x 1/2" x 1/2"

47.4

Market  

  • Construction

  • Bridges and highways

  • Chemical

  • Food and beverage

  • Manufacturing

  • Metals and mining

  • Microelectronics

  • Oil and gas

  • Pharmaceutical

  • Power

  • Pulp and paper

  • Leisure

  • Telecommunications

  • Transportation

  • Water and wastewater treatment

Features:

  • Corrosion-resistant

  • Low maintenance cost

  • Flame-retardant

  • Low installation cost

  • Heavy-metal safe

  • Long service life

  • Non-conductive, non-thermal-conductive

  • High strength-to-weight ratio

Raw material introduction — resin types

Code

Resin type

Flame-retardant performance

Recommended applications

VEFR-25

Vinyl ester type

Oxygen index 28 and above

Harsh acid, alkali and other corrosive environments

IFR-25

Isophthalic type

Oxygen index 28 and above

An economical VEFR type with excellent performance, resistant to moderate acids, alkalis and solvents

OFR-25

Orthophthalic type

Oxygen index 28 and above

General acid and alkali environments

  Applications: 

    Greenlogy TEC pultruded FRP profiles are widely used in various scenarios, combining corrosion resistance, high strength, dimensional stability and light weight, with thermal insulation and electrical insulation properties. Durable Greenlogy TEC profiles deliver years of low-maintenance service in applications where steel, aluminum or wood components have traditionally been specified. Today, these profiles are often used in highly corrosive applications that would otherwise require stainless steel and other costly components.    

Greenlogy TEC profiles

Mechanical properties

ASTM

Unit

Value

Unit

Value

Tensile stress, longitudinal

D-638

psi

30000

kgf/m²

21092086

Tensile stress, transverse

D-638

psi

7000

kgf/m²

4921487

Tensile modulus, longitudinal

D-638

10^6psi

2.5

10^6kgf/m²

1758

Tensile modulus, transverse

D-638

10^6psi

0.8

10^6kgf/m²

562

Compressive stress, longitudinal

D-695

psi

30000

kgf/m²

21092086

Compressive stress, transverse

D-695

psi

15000

kgf/m²

10546043

Compressive modulus, longitudinal

D-695

10^6psi

2.5

10^6kgf/m²

1758

Compressive modulus, transverse

D-695

10^6psi

1

10^6kgf/m²

703

Flexural stress, longitudinal

D-790

psi

30000

kgf/m²

21092086

Flexural stress, transverse

D-790

psi

10000

kgf/m²

7030695

Flexural modulus, longitudinal

D-790

10^6psi

1.8

10^6kgf/m²

1266

Flexural modulus, transverse

D-790

10^6psi

0.8

10^6kgf/m²

562

Modulus of elasticity

Full section

10^6psi

2.8

10^6kgf/m²

1969

Shear modulus

---

10^6psi

0.45

10^6kgf/m²

316

Short-beam shear

D-2344

psi

4500

kgf/m²

3163813

Punch shear

D-732

psi

10000

kgf/m²

7030695

Notched Izod impact strength, LW

D-256

ft.-lbs./in.

25

kg/m

3.46

Notched Izod impact strength, CW

D-256

ft.-lbs./in.

4

kg/m

0.55

 Excluding round rods and square rods 

Physical Properties

ASTM

Unit

Value

Barcol hardness

D-495

---

45

24-hour water absorption

D-570

%max

0.45

Density

D-792

lbs./in.³

0.062-0.07

Coefficient of thermal expansion, LW

D-696

10^-6in./in./℃

8

Flame-retardant performance

ASTM

Unit

Value

Tunnel test*

E-84

Flame spread

25 max

Flame resistance*

D-635

---

Non-combustible

Electrical properties

ASTM

Unit

Value

Arc resistance, LW

D-495

秒(s)

120

Dielectric strength, LW

D-149

kv./in.

35

Dielectric strength, PF

D-149

Volts/mil

200

Dielectric constant, PF

D-150

@60hz

5

LW = lengthwise, CW = crosswise, PF = perpendicular to laminate surface

*Applies to ISOFR and VEFR only


Application scenarios

Structural Profile - H Beam (Isophthalic) is suitable for applications with high requirements for corrosion resistance and strength, such as chemical platforms, wastewater treatment facilities, marine engineering, bridge walkways and long-span support structures. Its lightweight, high-strength characteristics reduce the load on support structures and facilitate installation and maintenance.

Selection Guide

When selecting, clarify the span, load conditions and service environment, and choose the appropriate cross-section size based on the existing specification table. If custom cross-sections or special lengths are required, please contact us for detailed specifications and quotations.

Product Advantages

The isophthalic resin system gives the product excellent corrosion resistance and water resistance, while glass fiber reinforcement ensures high strength and stiffness. The product is also lightweight, insulating, non-magnetic and long-lasting, making it suitable as a replacement for traditional metal profiles.

Inquiry Guidance

For detailed specifications, technical parameters or bulk purchase terms for Structural Profile - H Beam (Isophthalic), please contact us for detailed specifications and quotations. We will provide professional advice based on your needs.

Service Environment

  • This pultruded FRP H-beam is manufactured based on an isophthalic acid resin system, making the profile suitable for continuous use in outdoor and humid industrial environments where weak acids, weak bases and salt spray are present.
  • Glass fiber reinforcement and the isophthalic acid resin matrix enable this Structural Profile - H Beam (Isophthalic) to be used in chemical plants, wastewater treatment areas and coastal facilities, where steel requires frequent recoating or replacement.
  • Because the profile is non-conductive and corrosion-resistant, it is commonly selected for indoor and outdoor structural frames, platforms and support beams exposed to weather, moisture and process spills.
  • For applications involving concentrated chemicals, high temperatures or sustained loads at elevated temperatures, please contact us with the specific media and service conditions so that the correct resin grade and profile specification can be confirmed.