Product Category

Structural Profiles - Hollow Profile (Isophthalic)


Contact us for a quotation

Product details

Greenlogy TEC

   FRP pultruded profiles are a new type of composite material made from glass fiber reinforcement as the raw material, resin as the binder, and glass fiber cloth as the outer reinforcing layer. After thorough impregnation, the material is heated, formed and cured in a metal mold and then pulled by a pultrusion machine. With good physical properties, it is widely used in high-strength and long-span applications.   

Type

Size (mm)

Weight (kg/m)

Size (in)

Weight (lbs/in)

Hollow Profile

A1*T1*A2*T2*B*T3
A1*T1*A2*T2*B*T3

500*6*450*6*48.5*616.4

20" x 1/4" x 18" x 1/4" x 2" x 1/4"

36.2

500*6*450*6*48.5*918.5

20" x 1/4" x 18" x 1/4" x 2" x 3/8"

40.8

650*13*550*13*98.5*1252.5

51/2" x 1/2" x 173/8" x 1/2" x 4" x 1/2"

116

725*4.5*675*4.5*45*4.517.9

57/2" x 3/16" x 53/2" x 3/16" x 7/4" x 3/16"

39.5

Markets 

  • Construction

  • Bridges and highways

  • Chemical

  • Food and beverage

  • Manufacturing

  • Metals and mining

  • Microelectronics

  • Oil and gas

  • Pharmaceutical

  • Power

  • Pulp and paper

  • Leisure

  • Telecommunications

  • Transportation

  • Water and wastewater

Features:

  • Corrosion resistance

  • Low maintenance

  • Flame retardant

  • Low installation cost

  • Heavy-metal resistant

  • Long service life

  • Non-conductive, non-thermal-conductive

  • High strength-to-weight ratio

Raw material introduction — resin types

Code

Resin type

Flame retardancy

Recommended applications

VEFR-25

Vinylester type

Oxygen index 28 and above

Acid, alkali and other harsh corrosive environments

IFR-25

Isophthalic type

Oxygen index 28 and above

VEFR type: economical, good performance, moderate acid/alkali and solvent resistance

OFR-25

Orthophthalic type

Oxygen index 28 and above

General acid and alkali environments

Applications:   

   Greenlogy TEC pultruded fiberglass structural profiles are used in a wide range of applications, combining corrosion resistance, high strength, dimensional stability and light weight with thermal insulation and non-conductive properties. Durable Greenlogy TEC profiles provide years of low-maintenance service in areas where steel, aluminum or wood components are traditionally specified. Today, these profiles are often used in highly corrosive applications that previously required stainless steel and other costly components.    

Greenlogy TEC profiles

Mechanical properties

ASTM

Unit

Value

Unit

Value

Tensile stress, longitudinal

D-638

psi

30000

kgf/m²

21092086

Tensile stress, transverse

D-638

psi

7000

kgf/m²

4921487

Tensile modulus, longitudinal

D-638

10^6psi

2.5

10^6kgf/m²

1758

Tensile modulus, transverse

D-638

10^6psi

0.8

10^6kgf/m²

562

Compressive stress, longitudinal

D-695

psi

30000

kgf/m²

21092086

Compressive stress, transverse

D-695

psi

15000

kgf/m²

10546043

Compressive modulus, longitudinal

D-695

10^6psi

2.5

10^6kgf/m²

1758

Compressive modulus, transverse

D-695

10^6psi

1

10^6kgf/m²

703

Flexural stress, longitudinal

D-790

psi

30000

kgf/m²

21092086

Flexural stress, transverse

D-790

psi

10000

kgf/m²

7030695

Flexural modulus, longitudinal

D-790

10^6psi

1.8

10^6kgf/m²

1266

Flexural modulus, transverse

D-790

10^6psi

0.8

10^6kgf/m²

562

Modulus of elasticity

Full section

10^6psi

2.8

10^6kgf/m²

1969

Shear modulus

---

10^6psi

0.45

10^6kgf/m²

316

Short-beam shear

D-2344

psi

4500

kgf/m²

3163813

Punch shear

D-732

psi

10000

kgf/m²

7030695

Notched Izod impact strength, LW

D-256

ft.-lbs./in.

25

kg/m

3.46

Notched Izod impact strength, CW

D-256

ft.-lbs./in.

4

kg/m

0.55

  Excluding round rods and square rods  

Physical properties

ASTM

Unit

Value

Barcol hardness

D-495

---

45

24-hour water absorption

D-570

% max

0.45

Density

D-792

lbs./in.³

0.062-0.07

Coefficient of thermal expansion, LW

D-696

10^-6in./in./℃

8

Flame retardancy

ASTM

Unit

Value

Tunnel test*

E-84

Flame spread

Max. 25

Flame resistance*

D-635

---

Non-combustible

Electrical properties

ASTM

Unit

Value

Arc resistance, LW

D-495

秒(s)

120

Dielectric strength, LW

D-149

kv./in.

35

Dielectric strength, PF

D-149

Volts/mil

200

Dielectric constant, PF

D-150

@60hz

5

LW = lengthwise, CW = crosswise, PF = perpendicular to laminate surface

*Applies to ISOFR and VEFR only


Application Scenarios

The structural hollow profile (isophthalic) is suitable for load-bearing and support structures with requirements on strength and span, such as platform walkways, stair treads, handrails, cable tray supports, and frame members in corrosive environments such as chemical, marine and municipal facilities. Its hollow section maintains section stiffness while facilitating splicing and cut-out installation. To confirm whether it suits your specific application, please contact us with your operating conditions.

Selection Guide

When selecting, first determine the section height and wall thickness based on span, load and support method, then choose the cut-out or splicing solution according to the connection form of the installation node; the isophthalic resin system is suitable for environments with high corrosion resistance requirements and can be further discussed based on the medium and temperature conditions. The specifications listed on the page are common references; for actual dimensions, weight and mechanical parameters, please contact us for detailed specifications and a quotation.

Product Advantages

This profile uses glass fiber as reinforcement and resin as matrix and is formed by impregnation, heating, compression molding and curing with continuous pulling; it features light weight, high strength, corrosion resistance, non-magnetic properties, electrical insulation and ease of processing, cutting and drilling. The hollow profile structure achieves a larger section moment of inertia with the same material usage, making it suitable for high-strength, long-span support requirements. Contact us for information on the material system and process.

Inquiry Guidance

If you need to confirm requirements such as section dimensions, length, color, surface treatment, packaging and transportation, please contact us for detailed specifications and a quotation; we will recommend suitable specifications and supply solutions according to your project conditions. Bulk procurement, custom sections and technical selection support can all be discussed together.

Service Environment

  • These FRP pultruded hollow profiles use glass fiber as reinforcement and resin as bonding matrix; the finished structural profiles are suitable for outdoor and indoor service environments where moisture and atmospheric exposure persist—including walkways, platforms and structural frames exposed to the weather.
  • The isophthalic resin system used in this hollow profile grade makes it suitable for installation sites with corrosive media, such as chemical plants, wastewater treatment areas and coastal or seaside sites, where steel profiles require frequent coating maintenance.
  • Because the profile is cured in a heated metal mold and formed by continuous pulling, the hollow profile maintains its section across the service temperature range from normal ambient conditions to high-temperature plant environments; specific temperature and chemical resistance limits should be confirmed with us for each medium and concentration.
  • The hollow core also keeps weight low, making it suitable for long-span handrails, grating supports and platform frame members installed in high-humidity or washdown areas; before selecting A1*T1*A2*T2*B*T3 hollow profile for a specific environment, please contact Greenlogy TEC for the complete parameter table.