Product Category

Structural Profiles - Stair Tread Flat Tube (Isophthalic)


Contact us for a quotation

Product details

Greenlogy TEC

  FRP pultruded profiles are made from glass fiber reinforcement as the raw material, resin as the binder, and glass fiber cloth as the wrapping reinforcement layer. After full impregnation, they are heated, formed and cured in a metal mold and pulled out by a pulling machine. This new type of composite material has good physical properties and is widely used in high-strength and long-span applications.  

Type

Size (mm)

Weight (kg/m)

Size (in)

Weight (lbs/in)

Stair Tread Flat Tube

A*B*T1*T2


A*B*T1*T2


FT51A51*25*4*41.012" x 1" x 3/16" x 3/16"2.23
FT51B51*38*4*41.222" x 3/2" x 3/16 x 3/162.69
FT5252*32*5*51.412" x 5/4" x 3/16" x 3/16"3.11

Markets  

  • Construction

  • Bridges and highways

  • Chemical

  • Food and beverage

  • Manufacturing

  • Metals and mining

  • Microelectronics

  • Oil and gas

  • Pharmaceutical

  • Power

  • Pulp and paper

  • Recreation

  • Telecommunications

  • Transportation

  • Water and wastewater

Features:

  • Corrosion resistance

  • Low maintenance

  • Flame retardant

  • Low installation cost

  • Heavy metal resistant

  • Long service life

  • Non-conductive and non-thermal-conductive

  • High strength-to-weight ratio

Raw material introduction — resin types

Code

Resin type

Flame retardant performance

Recommended applications

VEFR-25

Vinyl ester type

Oxygen index 28 and above

Harsh corrosive environments such as acids and alkalis

IFR-25

Isophthalic type

Oxygen index 28 and above

VEFR type: economical, with good, moderate resistance to acids, alkalis and solvents

OFR-25

Orthophthalic type

Oxygen index 28 and above

General acid and alkali environments

Applications:

  Greenlogy TEC pultruded FRP structural profiles combine corrosion resistance, high strength, dimensional stability and light weight, with thermal insulation and electrical insulation properties. Durable Greenlogy TEC profiles provide years of low-maintenance service in areas where steel, aluminum or wood components are traditionally specified. Today, these profiles are often used in highly corrosive applications that previously required stainless steel and other costly components.  

Greenlogy TEC profiles

Mechanical properties

ASTM

Unit

Value

Unit

Value

Tensile stress, LW

D-638

psi

30000

kgf/m²

21092086

Tensile stress, CW

D-638

psi

7000

kgf/m²

4921487

Tensile modulus, LW

D-638

10^6psi

2.5

10^6kgf/m²

1758

Tensile modulus, CW

D-638

10^6psi

0.8

10^6kgf/m²

562

Compressive stress, LW

D-695

psi

30000

kgf/m²

21092086

Compressive stress, CW

D-695

psi

15000

kgf/m²

10546043

Compressive modulus, LW

D-695

10^6psi

2.5

10^6kgf/m²

1758

Compressive modulus, CW

D-695

10^6psi

1

10^6kgf/m²

703

Flexural stress, LW

D-790

psi

30000

kgf/m²

21092086

Flexural stress, CW

D-790

psi

10000

kgf/m²

7030695

Flexural modulus, LW

D-790

10^6psi

1.8

10^6kgf/m²

1266

Flexural modulus, CW

D-790

10^6psi

0.8

10^6kgf/m²

562

Modulus of elasticity

Full section

10^6psi

2.8

10^6kgf/m²

1969

Shear modulus

---

10^6psi

0.45

10^6kgf/m²

316

Short-beam shear

D-2344

psi

4500

kgf/m²

3163813

Punch shear

D-732

psi

10000

kgf/m²

7030695

Notched Izod impact strength, LW

D-256

ft.-lbs./in.

25

kg/m

3.46

Notched Izod impact strength, CW

D-256

ft.-lbs./in.

4

kg/m

0.55

  Excluding round rods and square rods

Physical properties

ASTM

Unit

Value

Barcol hardness

D-495

---

45

24-hour water absorption

D-570

% max

0.45

Density

D-792

lbs./in.³

0.062-0.07

Coefficient of thermal expansion, LW

D-696

10^-6in./in./℃

8

Flame retardant performance

ASTM

Unit

Value

Tunnel test*

E-84

Flame spread

Max 25

Flame resistance*

D-635

---

Non-burning

Electrical properties

ASTM

Unit

Value

Arc resistance, LW

D-495

秒(s)

120

Dielectric strength, LW

D-149

kv./in.

35

Dielectric strength, PF

D-149

Volts/mil

200

Dielectric constant, PF

D-150

@60hz

5

LW = lengthwise, CW = crosswise, PF = perpendicular to laminate surface

*Applies to ISOFR and VEFR only


Application Scenarios

The stair tread flat tube (isophthalic) is suitable for industrial platforms, stair treads, walkways and other locations requiring slip resistance and corrosion resistance. Its structural design facilitates the installation of anti-slip grit or grating panels, enhancing safety. Please contact us for specific application solutions.

Selection Guide

When selecting, consider factors such as load requirements, span and corrosive environment, and refer to the flat tube's dimensions and weight parameters. Isophthalic resin offers better corrosion resistance and is suitable for harsh environments such as chemical plants. For technical support, please contact us.

Product Advantages

Made with isophthalic resin, it offers excellent corrosion resistance and mechanical strength; glass fiber reinforcement ensures high load-bearing capacity; lightweight and high-strength for easy installation; insulating and non-magnetic, suitable for a variety of industrial environments.

Inquiry Guide

For detailed specifications, quotations or customization services, please contact us for more information. We provide professional technical support and prompt response.

Service Environment

  • This structural profile is produced with an isophthalic resin system, a formulation selected specifically for FRP components subjected to wet and chemical exposure conditions, making it suitable for both indoor plant environments and outdoor installations.
  • Typical use is as a stair tread flat tube on FRP walkways, platforms and tread boards, where the profile bears foot traffic and is continuously exposed to weather, washdown water and atmospheric moisture.
  • Pultruded glass fiber reinforced material using resin as the adhesive and glass fiber cloth as the wrapping reinforcement layer enables this flat tube to be used in corrosive industrial environments such as chemical plants, wastewater treatment areas, and marine and coastal locations, where steel requires coating or replacement.
  • Because the resin is corrosion-resistant and the composite material does not rust, the profile maintains its function under the temperature fluctuations and repeated wetting conditions typical of outdoor and process area use; for project-specific media and conditions, please contact the supplier for the full parameter table.