    FRP structural shapes profile is made of glass fiber reinforced material, resin as adhesive, glass fiber cloth as a package reinforcement layer, through the thorough penetration, in the metal mold heating, molding, curing, drawing in the traction machine pulled A new type of composite material, with good physical properties, widely used in high strength, large span Situation.  

Varieties

Size(mm)

Weight(kg/m)

Size(in)

Weight(lbs/in)

Plum tube

D1*D2*T


D1*D2*T


CT32A

19*32*6.4

1.11

3/4" x 5/4" x 1/4"

2.45

CT34A

19*34*7.5

1.3

3/4" x 5/4" x 5/16"

2.87

CT32B

25*32*3.5

0.66

1" x 5/4" x 1/8"

1.46

CT42

29*42*6.4

1.35

9/8" x 13/8" x 1/4"

2.98

CT45A

28*45*8.5

1.86

9/8" x 7/4" x 5/16"

4.1

CT45B

32*45*6.4

1.1

5/4" x 7/4" x 1/4"

2.43

CT51

51*36*7

1.75

2" x 3/2" x 1/4"

3.86

CT90B

71*90*9.5

5.7

11/4" x 7/2" x 3/8"

12.6

Markets  

  • Architectural

  • Bridge & Highway

  • Chemical

  • Food & Beverage

  • Manufacturing

  • Metals & Mining

  • Microelectronics

  • Oil & Gsa

  • Pharmaceutical

  • Power

  • Pulp & Paper

  • Recreation

  • Telecommunications

  • Transportation

  • Water & Wastewater

The characteristics:

  • Corrosion Resistant

  • Low Maintenance

  • Fire Retardant

  • Low Install Cost

  • Heavy Metal Safe

  • Long Service Life

  • Electrically & Thermally Non Conductive

  • High Strength-to-Weight Ratio

Introduction of raw materials——Resin type

Code

Resin type

Flame retardant property

Recommended usage occasions

VEFR-25

Vinyl type

Oxygen index 28 or above

Acid, alkali and other corrosive harsh environment

IFR-25

Meta benzene

Oxygen index 28 or above

A VEFR type economy, and excellent, moderate acid alkali and solvent

OFR-25

Ortho type

Oxygen index 28 or above

General acid and alkali environment

  Application:  

   Genius© pultruded fiberglass structural shapes from Genius Composite Inc. are used in a wide range of applications and provide a unique combination of corrosion resistance, high strength, dimensional stability and light weight, along with thermal and electric non-conductivity. Durable Genius shapes provide years of low maintenance service in areas where steel, aluminum or wood components are traditionally specified. Today ,these shapes are often used in highly corrosive applications where stainless steel and other expensive components were once required.   

Genius Shapes

Mechanical Properties

ASTM

Units

Value

Units

Value

Tensile Stress, LW

D-638

psi

30000

kgf/m²

21092086

Tensile Stress, CW

D-638

psi

7000

kgf/m²

4921487

Tensile Modulus, LW

D-638

10^6psi

2.5

10^6kgf/m²

1758

Tensile Modulus, CW

D-638

10^6psi

0.8

10^6kgf/m²

562

Compressive Stress, LW

D-695

psi

30000

kgf/m²

21092086

Compressive Stress, CW

D-695

psi

15000

kgf/m²

10546043

Compressive Modulus, LW

D-695

10^6psi

2.5

10^6kgf/m²

1758

Compressive Modulus, CW

D-695

10^6psi

1

10^6kgf/m²

703

Flexural Stress, LW

D-790

psi

30000

kgf/m²

21092086

Flexural Stress, CW

D-790

psi

10000

kgf/m²

7030695

Flexural Modulus, LW

D-790

10^6psi

1.8

10^6kgf/m²

1266

Flexural Modulus, CW

D-790

10^6psi

0.8

10^6kgf/m²

562

Modulus of Elasticity

Full Section

10^6psi

2.8

10^6kgf/m²

1969

Shear Modulus

---

10^6psi

0.45

10^6kgf/m²

316

Short Beam Shear

D-2344

psi

4500

kgf/m²

3163813

Punch Shear

D-732

psi

10000

kgf/m²

7030695

Notched Izod Impact,LW

D-256

ft.-lbs./in.

25

kg/m

3.46

Notched Izod Impact,CW

D-256

ft.-lbs./in.

4

kg/m

0.55

  Excludes Round Rod and Square Bar

Physical Properties

ASTM

Units

Value

Barcoal

D-495

---

45

24 Hour Water Absorption

D-570

%max

0.45

Density

D-792

lbs./in.³

0.062-0.07

Coefficient of Thermal Expansion,LW

D-696

10^-6in./in./℃

8

Flammability Properties

ASTM

Units

Value

Tunnel test*

E-84

Flame Spread

25 max

Flammability*

D-635

---

Non-Burning

Electrical Properties

ASTM

Units

Value

Arc Resistance,LW

D-495

seconds

120

Dielectric Strength,LW

D-149

kv./in.

35

Dielectric Strength,PF

D-149

volts/mil

200

Dielectric Constant,PF

D-150

@60hz

5

LW=Lengthwise, CW=Crosswise,PF=Perpendicular to Laminate Face

*Pertains to ISOFR and VEFR only


Application Scenarios

The quatrefoil tube structural profile combines strength with corrosion resistance, making it suitable for load-bearing supports and walkway frameworks in chemical platforms, wastewater treatment, power facilities, marine engineering and similar scenarios, with stable performance in humid, acid-base or salt-spray environments. For application-specific recommendations, please contact us for technical selection support.

Selection Guide

When selecting, consider load type, span, support spacing and environmental corrosion level, and confirm whether the cross-section dimensions (D1*D2*T) and wall thickness match installation requirements; weight parameters can also be referenced to estimate structural load. If you have questions about dimensions or mechanical properties, please contact us for detailed specifications and selection advice.

Product Advantages

This quatrefoil tube is pultruded from glass fiber reinforced resin, offering advantages such as lightweight and high strength, corrosion resistance, insulation and non-magnetic properties, and maintenance-free operation, along with easy installation that effectively reduces long-term use costs. To learn more about its technical features, please contact us to request samples and documentation.

Inquiry Guide

For detailed specifications, bulk pricing, delivery lead times or customization requirements, please contact us; we will provide professional advice and a quotation based on your application scenario.