Product Category

Product details

Greenlogy TEC  

FRP molded grating is a panel with a certain open area, made in custom molds with unsaturated polyester resin (including isophthalic, orthophthalic, phenolic and bisphenol types) as the matrix.

Name

Content

Type

Resin

35%

OFR-25,IFR-25,VEFR-25

Glass fiber

33%

E

Filler

31%

ATH,PR

Others

1%

---

Raw material introduction

Resin type

Code

Resin type

Flame retardancy

Recommended applications

MP-5

Phenolic type

Oxygen index up to approximately 80

Low toxicity, high flame retardancy; applications with high fire safety requirements

VEFR-25

Vinyl ester type

Oxygen index of 28 and above

Harsh corrosive environments such as acids and alkalis

VEFR-10

Vinyl ester type

Oxygen index of 35 and above

Applications with high acid/alkali and flame-retardant requirements and favorable service conditions

IFR-25

Isophthalic type

Oxygen index of 28 and above

VEFR type, economical and good, with moderate acid, alkali and solvent resistance

IFGR-30

benzene-type, food grade

oxygen index 26

mainly used in meat processing and food processing plants

OFR-25

orthophthalic type

Oxygen index of 28 and above

general acid and alkali environments

OCR

orthophthalic type

oxygen index below 28

OFR-25 economical type, no flame retardancy requirement

coarse glass fiber selection 

Codecoarse grit typeRecommended applications

E

E-glass grit

for high-strength requirements and highly corrosive environments

select filler type 

Code

filler type

Recommended applications

ATH

aluminum hydroxide

flame-retardant, smoke-suppressing and corrosion-resistant applications

PR

no filler, pure resin

for highly corrosion-resistant applications

channel type

Polished type

Workshop sand mold

38*38*30(mm)

Available panel size:

1524*4000,1220*4000,1220*3660,

1220*2440,915*3050 Load-bearing in both directions.     

Load-bearing flat bar thickness (top/bottom): 6.0/5.0

Load-bearing flat bar center distance: 38

Open area: 68%

Approx. weight: 14.6 kgs/m²

Line load (unit: mm)

Deflection



kg/m




Ultimate 

Span
(mm)

751503004507501500

Load

300<0.25<0.250.250.510.761.529923
4500.250.511.021.522.543.924828
6000.511.272.293.565.847.384112
7501.272.544.837.3712.516.03174
9002.274.549.0813.618.722.12637

Uniformly distributed load (unit: mm)

Deflection



kg/m²




Span
(mm)

350500750100015002500
3000.290.480.570.751.151.82
4500.781.191.812.473.544.95
6001.762.664.285.568.4113.2
7503.485.128.2111.016.42---
9005.898.8114.218.9------

Features:

  1. Corrosion resistant 

  2. Slip resistant 

  3. Ergonomic 

  4. Low installation cost 

  5. Flame retardant 

  6. Lightweight with high bidirectional strength; cutting makes the tubing easier to install.

  7. Uniform color inside and out; color can be selected freely.

  8. Offers favorable social and economic benefits.

  9. Excellent design flexibility, flexible and varied dimensions, dimensionally stable

 

Widely used in:

Greenlogy TEC FRP grating is widely used for industrial platform floors, stairways, walkways and platforms. Using FRP grating offers many advantages: good weather resistance, low maintenance cost, long service life and good anti-slip performance. In addition, FRP grating is simple, fast and flexible to fabricate and assemble.


Application scenarios

FRP molded grating 38*38H30 is suitable for platforms, walkways, trench covers and various industrial operating surfaces that require anti-slip performance, corrosion resistance and load bearing. Its mesh structure facilitates drainage, ventilation and light transmission, and is commonly used in chemical, water treatment, power and marine engineering environments. Contact us to confirm suitability for your specific operating conditions.

Selection guide

When selecting, please consider the resin system, load-bearing direction, support span and installation method, and make a comprehensive judgment based on media corrosiveness, ambient temperature and fire protection requirements. Different resin types have different strengths in corrosion resistance and flame retardancy, and should be matched to the actual application. Contact us for detailed specifications and selection advice.

Product advantages

Molded grating is integrally formed, with uniform fiber and resin distribution, combining lightweight, high strength, corrosion resistance and anti-slip performance, and is easy to cut and install on site. The surface can be treated for anti-slip, and long-term maintenance costs are relatively low. Contact us to learn about the performance characteristics of different resin systems.

Inquiry guidance

To confirm the resin type, color, dimensions and supply plan for 38*38H30 molded grating, please contact us. Please provide information such as the operating environment, load requirements and quantity, and we will provide specification recommendations and a quotation accordingly.